| Name | Value | Unit |
|---|---|---|
| Target Thickness | nm |
| Name | Value | Unit |
|---|---|---|
| NH3 Flow | 10 | cubic cm per min (sccm) |
| Pressure | 200 | mTorr |
| SiCl2H2 Flow | 80 | cubic cm per min (sccm) |
| Temperature | 825 | C |
| Name | Value | Unit | Confidence | Data Origin |
|---|---|---|---|---|
| Dep Rate | 4.65 | nm/min | 90 | This is an average of deposition rates from nine runs of Low Stress Nitride beginning Feb 6, 2025 through Dec 11 2025. Max dep rate of these was 4.9nm/min and min was 4.5nm/min. |
| Note | Date Modified | Author |
|---|---|---|
| Total Estimated Dep Time includes pull to load, push, pump down, temp ramp up, dep time, temp ramp down, vent, and pull to unload. Plan for additional time to measure thickness and enter data into HSC. | 2025-01-09 21:54:06 | anonymous |